For years the community has been speculating about the slight radioactivity of the early Minolta MC 1.2/58mm lenses. The values measured were far too low for a "real" thorium glass, especially since all lenses inside the MC 1.2/58mm are pretty large. In addition the slight (very slight indeed) yellowing of the lens isn't in accordance with the behaviour of genuine thorium glass.

I myself have speculated that some thorium impurities in the lanthanum glass might be responsible, but there's another explanation.

OK, some background here: Minolta has always been on the forefront of coating, and especially of multicoating; in fact they were the first to coat lenses in Japan (1944), and the first to introduce double coating in 1957. Just when the other Japanese manufacturers started to introduce double coating (around 1965-70), Minolta was developing a four layer coating. It was patented in Japan and Germany, but not in the US.

The German patent lists the following components for the first and the fourth layer:
MgF2 (1.385), SiO2 (1.46), ThF4 (1.5) and others ... bingo: Thorium fluoride!

For the second layer some high refractive materials are used, e. g.
CeO2, ZrO2, TiO2 (all in the 2.0-2.3 range) and ... thorium oxide ThO2 (v=2.3)!

And for the third layer - among others - thorium hydroxide ThOH2 is suggested ...

Here we are - this explains the traces of radioactivity as well as as the traces of yellowing on 1st gen Minolta MC 1.2/58mm lenses.

And why only the MC 1.2/58, and not the other multicoated Minolta lenses from around 1970? Well, Minolta-related experts such as the engineer Josef Scheibel and the writer Dieter Gabler were - back in the days - pretty vocal about the fact that Minolta was choosing the optimal multicoating for each air-glass surface individually, thus fine-tuning it to the corresponding glass used.

Source: DE2334875

Mystery solved, methinks ...

S


最后由 stevemark 于 周三 6月 25, 2025 11:12 am 编辑;共编辑 1 次


Reply

Nice work.


Reply

Very interesting Stephan!!

Do you think this may also apply to the MC Rokkor 28mm/2.5? They are reported to be radioactive; all three samples I have were slightly yellowed, and all responded well to UV exposure for a few days to eliminate the colour cast, with the offending lens group extracted and exposed in a UV radiation box. Maybe for that lens there is a similar issue of thorium used in the coatings rather than thorium used in the glass?


Reply

I am firmly convinced that this interpretation is not correct.

Maury Jacks has measured radioactivity at the rear of these lenses at close to 8 uSv/hr, which is exactly in line with Hexanons known to contain radioactive glass, and it's not far (well within an order of magnitude) from what you see in the known highly-radioactive/very prone to yellowing Super Takumar 50mm f/1.4 (around 22 uSv/hr), a lens that uses a very similar 7 element double Gauss design.

I also can anecdotally say from my own disassemblies of this lens that it is indeed primarily the glass of a specific element that yellows in them, IIRC 3rd from the rear, the biconvex half of the cemented achromatic doublet. This unsurprisingly corresponds to exactly the same position of the radioactive element in the Takumars, which replaced two elements of the cemented triplet in the original 8 element Takumar design. This doesn't rule out radioactive coatings being present as well, but if they were behind the yellowing, one would expect to see the same degree across each of the elements.

It's also worth noting that the yellowing is consistent through the entire fabric of the affected element. If this were a case of coatings being chosen individually, presumably the air gapped and cemented sides of the element would be using drastically different coatings, yet there is no difference in the yellowing that either side of the glass fabric displays. Likewise, the same degree of yellowing would presumably be seen at the adjoining surface of the element cemented directly to the theorized radioactive coating. It does not, only sometimes showing very mild yellowing, which also leads me to believe it is indeed the glass fabric of the affected element that is emitting the radiation rather than the coatings.

(The second from rear element also sometimes shows a somewhat lesser degree of yellowing, presumably from being immediately adjacent to the radioactive one or from being mildly radioactive itself.)

Here's an image showing the position of the yellowing element in the Minolta:



Also worth adding Jacks put together a chart that he has posted on the link below showing various degrees of yellowing.


He has admittedly boosted the saturation on the image, but as you can see, particularly in the first lens on row 2, the yellowing can be pretty substantial in these.


Reply

RokkorDoctor 写道:
Very interesting Stephan!!

Do you think this may also apply to the MC Rokkor 28mm/2.5? They are reported to be radioactive; all three samples I have were slightly yellowed, and all responded well to UV exposure for a few days to eliminate the colour cast, with the offending lens group extracted and exposed in a UV radiation box. Maybe for that lens there is a similar issue of thorium used in the coatings rather than thorium used in the glass?


No, certainly not. The MC 2.5/28 has a much, much stronger yellowing than the early 1.2/58mm lenses, even though its radioactive lens (at the rear) is much smaller than any of the seven lenses of the MC 1.2/58mm. The yellowing and the radioactivity of the MC 2.5/28mm are similar to that of the radioactive Takumar 1.4/50mm ...



BrianSVP 写道:

Maury Jacks has measured radioactivity at the rear of these lenses at close to 8 uSv/hr, which is exactly in line with Hexanons known to contain radioactive glass, and it's not far (well within an order of magnitude) from what you see in the known highly-radioactive/very prone to yellowing Super Takumar 50mm f/1.4 (around 22 uSv/hr), a lens that uses a very similar 7 element double Gauss design.

I wasn't aware of these relatively high values - the values I occasionally had read were much lower.

BrianSVP 写道:
I also can anecdotally say from my own disassemblies of this lens that it is indeed primarily the glass of a specific element that yellows in them, IIRC 3rd from the rear, the biconvex half of the cemented achromatic doublet. .... This doesn't rule out radioactive coatings being present as well, but if they were behind the yellowing, one would expect to see the same degree across each of the elements.

Not necessarily. If you look at Minolta glass from that time frame, you easily can spot the different coatings applied to each element within a single objective (some brownish, some greenish, some blueish). That - as well as the German literature I've cited in my above posting - prove that Minolta was choosing the coating individually for each single glass element.

BrianSVP 写道:
It's also worth noting that the yellowing is consistent through the entire fabric of the affected element. If this were a case of coatings being chosen individually, presumably the air gapped and cemented sides of the element would be using drastically different coatings,
I'm not aware that the cemented sides of a single lens would ever be coated, since the refraction index of canada balsam is about 1.52 (same as crown glass) ... but I may be wrong ...


BrianSVP 写道:
yet there is no difference in the yellowing that either side of the glass fabric displays.

Just for clarification: You have split the corresponding doublet into its two parts, and looked at both surfaces of the big biconvex lens (yellow in your drawing)?


BrianSVP 写道:
Likewise, the same degree of yellowing would presumably be seen at the adjoining surface of the element cemented directly to the theorized radioactive coating.

No; there's usually no coating at all on the cemented glass surfaces.


I agree with you that the substatial radioactivity detected by Maury Jacks is indicating some thoriated glass. As I said I had much lower values in my mind (but can't immediately find those postings any more).

That said, my own MC-II 1.2/58mm (SN 2510663 and thus pretty early when looking at Maury Jacks' samples) has a very faint yellowing only (compared to the later MC-X 1.2/58mm), far less than the 1.4/50mm Takumars I own, and fare less than the MC 2.5/28mm as well. And to my eye this (weak) yellowing seems to be pretty uniform across the diameter of the lens (but agan: I may be wrong here). I would expect significantly more yellowing especially in the center if the glass itself was thoriated (lens is much thicker in the center than at its borders).

Nevertheless it seems the computation of the MC 1.2/58mm was modifed at some point since the lens sections pulished by Minolta have been changing slightly when going from MC-II to MC-X (look at both the front as well as at the rear doublets) - that againg would indicate a change from thoriated to non-thoriated glass, as you have suggested:
https://web.archive.org/web/20241217195245/http://www.artaphot.ch/minolta-sr/objektive/236-minolta-58mm-f12

S


Reply

I'm constantly amazed that I still can see no yellowing in my MC ROKKOR-PG 58mm f1.2 (#2580654).

Whatever the cause, this discussion has convinced me to Fuhgeddaboudit.


Reply

xkaes 写道:
I'm constantly amazed that I still can see no yellowing in my MC ROKKOR-PG 58mm f1.2 (#2580654).

Whatever the cause, this discussion has convinced me to Fuhgeddaboudit.



It has been established by Maury Jacks that the highest radioactive lens recorded bears serial No 2567714 so yours has a much higher SN and thus was made much later. That is why you see no yellowing.


Reply

I happened to acquire another one of these lenses today and pulled it apart in the course of CLA so you could see the evidence prior to deyellowing.

This is from an MC Rokkor-PG, SN#2508855. It is the earlier second version with metal knurled grip and flat headed mount screws.

These are the three rear groups of the lens, with the rearmost on the left and the innermost (the doublet) on the right.



As you can see, the doublet is pretty darn yellowed. This is about the same amount of yellowing as seen in the SMC Takumar 50mm f/1.4, and somewhat less than seen in the Super version of the same. The next element adjacent to it has just a tiny bit of yellowing, and the rearmost essentially none.

I've separated doublets like this in the past to recement, and I've observed that the yellowing is almost entirely in the crown (convex) side of the doublet, whereas the flint looks like the element in the middle, with just slight yellowing. The yellowing in the crown extends evenly through the entire fabric of the element, with even yellowing along the ground glass edge where the coating wouldn't be present.

It's worth noticing that the this position, the crown of the rear doublet, is where you most typically find the radioactive glass in most of the planar-derived derived designs that incorporate it, so finding it here is really no surprise at all.


Reply

BrianSVP 写道:
I happened to acquire another one of these lenses today and pulled it apart in the course of CLA so you could see the evidence prior to deyellowing.

This is from an MC Rokkor-PG, SN#2508855. It is the earlier second version with metal knurled grip and flat headed mount screws.

These are the three rear groups of the lens, with the rearmost on the left and the innermost (the doublet) on the right.

As you can see, the doublet is pretty darn yellowed. This is about the same amount of yellowing as seen in the SMC Takumar 50mm f/1.4, and somewhat less than seen in the Super version of the same. The next element adjacent to it has just a tiny bit of yellowing, and the rearmost essentially none.

I've separated doublets like this in the past to recement, and I've observed that the yellowing is almost entirely in the crown (convex) side of the doublet, whereas the flint looks like the element in the middle, with just slight yellowing. The yellowing in the crown extends evenly through the entire fabric of the element, with even yellowing along the ground glass edge where the coating wouldn't be present.

It's worth noticing that the this position, the crown of the rear doublet, is where you most typically find the radioactive glass in most of the planar-derived derived designs that incorporate it, so finding it here is really no surprise at all.


Good information! It looks like from the angle of the pic that the lens has uneven yellowing, or is it separated? I have never worked on one of these, but I need one for sure! Smile All of my radioactive Takumars and others do seem to be the most yellowed in the center as you mentioned. Also, not to get too off topic, but what do you use to re-cement the elements? I have a few that need to be redone, but it is hard to find a UV glue that is generally not more expensive than the lens I am working on.


Reply

Kenolta 写道:

Good information! It looks like from the angle of the pic that the lens has uneven yellowing, or is it separated? I have never worked on one of these, but I need one for sure! Smile All of my radioactive Takumars and others do seem to be the most yellowed in the center as you mentioned. Also, not to get too off topic, but what do you use to re-cement the elements? I have a few that need to be redone, but it is hard to find a UV glue that is generally not more expensive than the lens I am working on.


(Apparent) stronger yellowing near the centre of a convex radioactive element makes sense. The colouring happens throughout the thorium glass body, not just on the surface. The convex lens element is thicker in the centre, hence more apparent colouration in the centre: the light has to pass through more of the coloured glass near the centre.

Conversely, in a concave thorium glass element you would expect the yellowing to be more apparent towards the edges, and less so in the centre because there the edges of the element are thicker than the centre.


Reply

I use Norland Optical Adhesive NOA 61. Edmund Scientific sells a preloaded syringe that would be enough for the lifetime of any hobbyist for less than US$30. They also sell a 1 oz bottle for about $40.There used to be a guy on eBay who sold tiny droppers of it for about $10, but I don't know if he is still around. He marketed it as binocular adhesive, but it's suitable for most optical projects and has a similar refractive index to Canada balsam.

It's the same stuff the U.S. military uses in its optics, so as you might imagine, it is pretty tough. Once cured under UV light, it's very difficult to get back apart, so it's a lot less forgiving than balsam, and you have to be very careful to get the elements centered and that you don't have any bubbles, debris, etc. before curing.

As far as the yellowing in the pic goes, the main yellowed doublet on the right is consistently yellowed throughout the entire element. If you're referring to the one in the middle, I think that might just be a weird reflection, since to the naked eye it doesn't look nearly as yellow, whereas the doublet is much more obviously yellowed.

Kenolta 写道:
BrianSVP 写道:
I happened to acquire another one of these lenses today and pulled it apart in the course of CLA so you could see the evidence prior to deyellowing.

This is from an MC Rokkor-PG, SN#2508855. It is the earlier second version with metal knurled grip and flat headed mount screws.

These are the three rear groups of the lens, with the rearmost on the left and the innermost (the doublet) on the right.

As you can see, the doublet is pretty darn yellowed. This is about the same amount of yellowing as seen in the SMC Takumar 50mm f/1.4, and somewhat less than seen in the Super version of the same. The next element adjacent to it has just a tiny bit of yellowing, and the rearmost essentially none.

I've separated doublets like this in the past to recement, and I've observed that the yellowing is almost entirely in the crown (convex) side of the doublet, whereas the flint looks like the element in the middle, with just slight yellowing. The yellowing in the crown extends evenly through the entire fabric of the element, with even yellowing along the ground glass edge where the coating wouldn't be present.

It's worth noticing that the this position, the crown of the rear doublet, is where you most typically find the radioactive glass in most of the planar-derived derived designs that incorporate it, so finding it here is really no surprise at all.


Good information! It looks like from the angle of the pic that the lens has uneven yellowing, or is it separated? I have never worked on one of these, but I need one for sure! Smile All of my radioactive Takumars and others do seem to be the most yellowed in the center as you mentioned. Also, not to get too off topic, but what do you use to re-cement the elements? I have a few that need to be redone, but it is hard to find a UV glue that is generally not more expensive than the lens I am working on.


Reply

I used the Norland Adhesive to (incorrectly) bond a doublet recently, it can be separated again by heating to roughly 180-200 degrees centigrade, which was successfully accomplished. Prior to this I soaked it in Acetone for 3-4 weeks with no result. Heating to separate is fraught with uncertainties. It the interface is curved and the glass type on the inside of the curve has a higher coefficient of expansion with heat than the outer element, catastrophic damage can occur.

Once separated the residue of the epoxy still needs to be removed, with some type of methylene chloride compound, or something slightly less cancer causing if possible.


Reply

An old trick to separate cemented doublets if you are daring/willing to risk the lens is to place it on top of an incandescent light bulb and turn it on, watching carefully until the cement separates - you'll see it as it happens!.

The plastic welder commonly used by model hobbyists (Micro Mark Same Stuff, etc.) can be brushed on to remove excess cement traces. It does contain methylene chloride and so should be used in a well ventilated space. Depending on what country you live in, it may or may not be legal to purchase.

Alun Thomas 写道:
I used the Norland Adhesive to (incorrectly) bond a doublet recently, it can be separated again by heating to roughly 180-200 degrees centigrade, which was successfully accomplished. Prior to this I soaked it in Acetone for 3-4 weeks with no result. Heating to separate is fraught with uncertainties. It the interface is curved and the glass type on the inside of the curve has a higher coefficient of expansion with heat than the outer element, catastrophic damage can occur.

Once separated the residue of the epoxy still needs to be removed, with some type of methylene chloride compound, or something slightly less cancer causing if possible.


Reply

BrianSVP 写道:

I use Norland Optical Adhesive NOA 61. Edmund Scientific sells a preloaded syringe that would be enough for the lifetime of any hobbyist for less than US$30. They also sell a 1 oz bottle for about $40.There used to be a guy on eBay who sold tiny droppers of it for about $10, but I don't know if he is still around. He marketed it as binocular adhesive, but it's suitable for most optical projects and has a similar refractive index to Canada balsam.

It's the same stuff the U.S. military uses in its optics, so as you might imagine, it is pretty tough. Once cured under UV light, it's very difficult to get back apart, so it's a lot less forgiving than balsam, and you have to be very careful to get the elements centered and that you don't have any bubbles, debris, etc. before curing.

An old trick to separate cemented doublets if you are daring/willing to risk the lens is to place it on top of an incandescent light bulb and turn it on, watching carefully until the cement separates - you'll see it as it happens!.

The plastic welder commonly used by model hobbyists (Micro Mark Same Stuff, etc.) can be brushed on to remove excess cement traces. It does contain methylene chloride and so should be used in a well ventilated space. Depending on what country you live in, it may or may not be legal to purchase.




Thanks, I will give the NOA 61 a try! I was imagining there would only be enough for one lens, but I guess it just takes a few drops. For the Canadian balsam cemented lenses I just use the oven along with some Ove Gloves to separate. Smile I will find or 3d print some v-blocks to align the lenses before using the UV light. It will hopefully be easy to rig something up.


Reply

https://youtu.be/VY1U4bOD2mo?t=516

In this video he claims Minolta used radioactive material for quite a while including into the MD lenses.